Spin Coating Curve Library

Find a starting spin speed for a common coating material. Compare sourced thickness curves, check the process conditions, and choose the next coating trial.

A starting reference for process development. These curves combine published supplier references and independent laboratory results. They are not Cee-validated recipes. Graph readings are approximate; older references and incomplete conditions are identified on each card. Thickness measurement stage, formulation, solvent, spin time, acceleration, substrate and exhaust must match for a meaningful comparison.

Where do I start with a recipe?

  1. Match the bottle. Select the exact product grade, molecular weight, concentration and solvent. A generic material name is not enough.
  2. Match the conditions. Open the source details and check spin time, substrate, dispense, acceleration and bake. Resolve missing information before using a reference as a recipe.
  3. Run and measure. Use the reference to choose a trial within your approved equipment and material limits. Measure thickness at a consistent process stage and map film uniformity.
  4. Build your local curve. Repeat at nearby speeds while holding the other variables consistent. Use your own measurements in the spin speed calculator.

Browse the curves

59 curves shown

Approximate graph readings

AZ 10XT · 220 cP

3.9–10.5 µm across 1000–5000 rpm · approximate

AZ 10XT · 220 cP spin speed versus thicknessApproximate graph readings. Merck, AZ 10XT technical datasheet; p. 1, spin curves; p. 12, coating notes. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_10xt_photoresist.pdf. 150 mm silicon. Distinct 220 cP and 520 cP grades; curves assume spinning to equilibrium. No fixed spin duration is specified. Do not transfer these curves to shortened spins or a different viscosity grade. Acceleration, exhaust and curve-specific bake are not specified.AZ 10XT · 220 cPApproximate graph readings · AZ manufacturer reference03.026.049.0612.110002000300040005000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm silicon. Distinct 220 cP and 520 cP grades; curves assume spinning to equilibrium. No fixed spin duration is specified.

Data, conditions and source

AZ 10XT, 220 cP viscosity grade

Reference data (µm)
rpmThickness ≈
100010.5
20006.5
30005.1
40004.4
50003.9

Do not transfer these curves to shortened spins or a different viscosity grade. Acceleration, exhaust and curve-specific bake are not specified.

Source: Merck, AZ 10XT technical datasheet. p. 1, spin curves; p. 12, coating notes. Revision March 2021; checked November 24, 2026.

Approximate graph readings

AZ 10XT · 520 cP

7.3–18.3 µm across 1000–5000 rpm · approximate

AZ 10XT · 520 cP spin speed versus thicknessApproximate graph readings. Merck, AZ 10XT technical datasheet; p. 1, spin curves; p. 12, coating notes. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_10xt_photoresist.pdf. 150 mm silicon. Distinct 220 cP and 520 cP grades; curves assume spinning to equilibrium. No fixed spin duration is specified. Do not transfer these curves to shortened spins or a different viscosity grade. Acceleration, exhaust and curve-specific bake are not specified.AZ 10XT · 520 cPApproximate graph readings · AZ manufacturer reference05.2610.515.82110002000300040005000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm silicon. Distinct 220 cP and 520 cP grades; curves assume spinning to equilibrium. No fixed spin duration is specified.

Data, conditions and source

AZ 10XT, 520 cP viscosity grade

Reference data (µm)
rpmThickness ≈
100018.3
200012.3
30009.5
40008.2
50007.3

Do not transfer these curves to shortened spins or a different viscosity grade. Acceleration, exhaust and curve-specific bake are not specified.

Source: Merck, AZ 10XT technical datasheet. p. 1, spin curves; p. 12, coating notes. Revision March 2021; checked November 24, 2026.

Approximate graph readings

AZ 12XT-20PL

8–20 µm across 1000–5000 rpm · approximate

AZ 12XT-20PL spin speed versus thicknessApproximate graph readings. Merck, AZ 12XT-20PL technical datasheet; p. 1, spin curve. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_12xt_photoresist.pdf. 150 mm silicon; AZ 12XT-20PL. Final spin duration is not stated. Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.AZ 12XT-20PLApproximate graph readings · AZ manufacturer reference05.7511.517.32310002000300040005000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm silicon; AZ 12XT-20PL. Final spin duration is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
100020
200014
300011
40009.3
50008

Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.

Source: Merck, AZ 12XT-20PL technical datasheet. p. 1, spin curve. Source checked November 24, 2026.

Approximate graph readings

AZ 40XT-11D

33–72 µm across 1000–3000 rpm · approximate

AZ 40XT-11D spin speed versus thicknessApproximate graph readings. Merck, AZ 40XT-11D technical datasheet; p. 1, spin curve. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_40xt_11d_photoresist.pdf. 200 mm silicon; hand dispense at 30 rpm; final spin 20 s; bake 125 °C for 7 min. Exhaust and acceleration are not stated. Thick-film results depend on both spin speed and duration.AZ 40XT-11DApproximate graph readings · AZ manufacturer reference020.741.462.182.8100020003000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

200 mm silicon; hand dispense at 30 rpm; final spin 20 s; bake 125 °C for 7 min.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
100072
150052
200043
250037
300033

Exhaust and acceleration are not stated. Thick-film results depend on both spin speed and duration.

Source: Merck, AZ 40XT-11D technical datasheet. p. 1, spin curve. Revision July 2016; checked November 24, 2026.

Approximate graph readings

AZ 1505

0.5–1.1 µm across 1000–4000 rpm · approximate

AZ 1505 spin speed versus thicknessApproximate graph readings. Merck, AZ 1500 Series technical datasheet; p. 1, spin curves. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_1500_series.pdf. 150 mm wafers. Final spin duration is not stated. Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.AZ 1505Approximate graph readings · AZ manufacturer reference00.3160.6320.9491.261000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm wafers. Final spin duration is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10001.1
20000.75
30000.6
40000.5

Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.

Source: Merck, AZ 1500 Series technical datasheet. p. 1, spin curves. Source checked November 24, 2026.

Original source
Approximate graph readings

AZ 1512

1.3–2.6 µm across 1000–4000 rpm · approximate

AZ 1512 spin speed versus thicknessApproximate graph readings. Merck, AZ 1500 Series technical datasheet; p. 1, spin curves. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_1500_series.pdf. 150 mm wafers. Final spin duration is not stated. Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.AZ 1512Approximate graph readings · AZ manufacturer reference00.7471.492.242.991000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm wafers. Final spin duration is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10002.6
20001.85
30001.5
40001.3

Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.

Source: Merck, AZ 1500 Series technical datasheet. p. 1, spin curves. Source checked November 24, 2026.

Approximate graph readings

AZ 1518

1.9–4.3 µm across 1000–4000 rpm · approximate

AZ 1518 spin speed versus thicknessApproximate graph readings. Merck, AZ 1500 Series technical datasheet; p. 1, spin curves. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_1500_series.pdf. 150 mm wafers. Final spin duration is not stated. Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.AZ 1518Approximate graph readings · AZ manufacturer reference01.242.473.714.941000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm wafers. Final spin duration is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10004.3
20002.8
30002.2
40001.9

Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.

Source: Merck, AZ 1500 Series technical datasheet. p. 1, spin curves. Source checked November 24, 2026.

Original source
Approximate graph readings

AZ 1529

3.3–8 µm across 1000–4000 rpm · approximate

AZ 1529 spin speed versus thicknessApproximate graph readings. Merck, AZ 1500 Series technical datasheet; p. 1, spin curves. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_1500_series.pdf. 150 mm wafers. Final spin duration is not stated. Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.AZ 1529Approximate graph readings · AZ manufacturer reference02.34.66.99.21000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm wafers. Final spin duration is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10008
20005.1
30004
40003.3

Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.

Source: Merck, AZ 1500 Series technical datasheet. p. 1, spin curves. Source checked November 24, 2026.

Original source
Published supplier values

AZ 5214E

1.14–1.98 µm across 2000–6000 rpm

AZ 5214E spin speed versus thicknessPublished supplier values. Merck, AZ 5214E technical datasheet; p. 2, characteristic thickness table. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_5214e_photoresist.pdf. AZ 5214E in PGMEA. The source does not state spin time or substrate dimensions for the table. Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.AZ 5214EPublished supplier values · AZ supplier table00.5691.141.712.2820003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

AZ 5214E in PGMEA. The source does not state spin time or substrate dimensions for the table.

Data, conditions and source
Reference data (µm)
rpmThickness
20001.98
30001.62
40001.4
50001.25
60001.14

Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.

Source: Merck, AZ 5214E technical datasheet. p. 2, characteristic thickness table. Source checked November 24, 2026.

Approximate graph readings

AZ 9260

6.3–15 µm across 1000–4500 rpm · approximate

AZ 9260 spin speed versus thicknessApproximate graph readings. AZ Electronic Materials, AZ 9260 data package (hosted by University of Utah); p. 4, film thickness versus spin speed. https://www.nanofab.utah.edu/wp-content/uploads/2022/12/AZ-9260-Thick-Positive-Photoresist-Spec-Sheet-1-1.pdf. Static dispense on 150 mm silicon; 30 s final spin. Proximity bake at 110 °C: 10 s at 0.050 inch, then 180 s at 0.002 inch. Acceleration and exhaust are not stated. Archived manufacturer reference; confirm current grade and supplier guidance.AZ 9260Approximate graph readings · AZ archived manufacturer reference04.318.6312.917.310002000300040004500Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Static dispense on 150 mm silicon; 30 s final spin. Proximity bake at 110 °C: 10 s at 0.050 inch, then 180 s at 0.002 inch.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
100015
150011.7
20009.9
25008.7
30007.9
35007.2
40006.7
45006.3

Acceleration and exhaust are not stated. Archived manufacturer reference; confirm current grade and supplier guidance.

Source: AZ Electronic Materials, AZ 9260 data package (hosted by University of Utah). p. 4, film thickness versus spin speed. Source checked November 24, 2026.

Published supplier values

AZ BARLi II 90

86–113 nm across 2000–3500 rpm

AZ BARLi II 90 spin speed versus thicknessPublished supplier values. Clariant/AZ, BARLi II technical brochure; p. 3, film-thickness table. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_barli_II.pdf. BARLi II 90 and II 200 are separate grades. Published thickness table in ångströms; converted here to nm (10 Å = 1 nm). Spin duration and table-specific substrate/bake conditions are not stated. The general brochure recommends a 200 °C, 60 s bake; do not assume that fully specifies the table process.AZ BARLi II 90Published supplier values · AZ supplier table032.56597.5130200030003500Spin speed (rpm)Film thickness (nm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

BARLi II 90 and II 200 are separate grades. Published thickness table in ångströms; converted here to nm (10 Å = 1 nm).

Data, conditions and source
Reference data (nm)
rpmThickness
2000113
2500101
300093
350086

Spin duration and table-specific substrate/bake conditions are not stated. The general brochure recommends a 200 °C, 60 s bake; do not assume that fully specifies the table process.

Source: Clariant/AZ, BARLi II technical brochure. p. 3, film-thickness table. Source checked November 24, 2026.

Published supplier values

AZ BARLi II 200

186–235 nm across 2000–3500 rpm

AZ BARLi II 200 spin speed versus thicknessPublished supplier values. Clariant/AZ, BARLi II technical brochure; p. 3, film-thickness table. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_barli_II.pdf. BARLi II 90 and II 200 are separate grades. Published thickness table in ångströms; converted here to nm (10 Å = 1 nm). Spin duration and table-specific substrate/bake conditions are not stated. The general brochure recommends a 200 °C, 60 s bake; do not assume that fully specifies the table process.AZ BARLi II 200Published supplier values · AZ supplier table067.6135203270200030003500Spin speed (rpm)Film thickness (nm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

BARLi II 90 and II 200 are separate grades. Published thickness table in ångströms; converted here to nm (10 Å = 1 nm).

Data, conditions and source
Reference data (nm)
rpmThickness
2000235
2500216
3000201
3500186

Spin duration and table-specific substrate/bake conditions are not stated. The general brochure recommends a 200 °C, 60 s bake; do not assume that fully specifies the table process.

Source: Clariant/AZ, BARLi II technical brochure. p. 3, film-thickness table. Source checked November 24, 2026.

Approximate graph readings

AZ MiR 701 · 14 cP

0.75–1.7 µm across 1000–6000 rpm · approximate

AZ MiR 701 · 14 cP spin speed versus thicknessApproximate graph readings. Merck, AZ MiR 701 Series technical datasheet; p. 1, spin curves. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_mir701_series.pdf. 150 mm wafers; separate 14 cP and 29 cP grades. Final spin duration is not stated. Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.AZ MiR 701 · 14 cPApproximate graph readings · AZ manufacturer reference00.4890.9771.471.95100020003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm wafers; separate 14 cP and 29 cP grades. Final spin duration is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10001.7
20001.2
30001
40000.9
60000.75

Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.

Source: Merck, AZ MiR 701 Series technical datasheet. p. 1, spin curves. Source checked November 24, 2026.

Approximate graph readings

AZ MiR 701 · 29 cP

1.3–3.1 µm across 1000–6000 rpm · approximate

AZ MiR 701 · 29 cP spin speed versus thicknessApproximate graph readings. Merck, AZ MiR 701 Series technical datasheet; p. 1, spin curves. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_mir701_series.pdf. 150 mm wafers; separate 14 cP and 29 cP grades. Final spin duration is not stated. Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.AZ MiR 701 · 29 cPApproximate graph readings · AZ manufacturer reference00.8911.782.673.56100020003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm wafers; separate 14 cP and 29 cP grades. Final spin duration is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10003.1
20002.2
30001.8
40001.6
60001.3

Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.

Source: Merck, AZ MiR 701 Series technical datasheet. p. 1, spin curves. Source checked November 24, 2026.

Approximate graph readings

AZ nLOF 2020

1.7–3.4 µm across 1000–4000 rpm · approximate

AZ nLOF 2020 spin speed versus thicknessApproximate graph readings. Merck, AZ nLOF 2000 Series technical datasheet; p. 1, spin curves. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_nlof2000_series.pdf. 150 mm silicon. Final spin duration is not stated. Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.AZ nLOF 2020Approximate graph readings · AZ manufacturer reference00.9771.952.933.911000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm silicon. Final spin duration is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10003.4
20002.4
30002
40001.7

Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.

Source: Merck, AZ nLOF 2000 Series technical datasheet. p. 1, spin curves. Source checked November 24, 2026.

Approximate graph readings

AZ nLOF 2035

2.8–5.8 µm across 1000–4000 rpm · approximate

AZ nLOF 2035 spin speed versus thicknessApproximate graph readings. Merck, AZ nLOF 2000 Series technical datasheet; p. 1, spin curves. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_nlof2000_series.pdf. 150 mm silicon. Final spin duration is not stated. Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.AZ nLOF 2035Approximate graph readings · AZ manufacturer reference01.673.3356.671000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm silicon. Final spin duration is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10005.8
20004
30003.25
40002.8

Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.

Source: Merck, AZ nLOF 2000 Series technical datasheet. p. 1, spin curves. Source checked November 24, 2026.

Original source
Approximate graph readings

AZ nLOF 2070

5.3–11 µm across 1000–4000 rpm · approximate

AZ nLOF 2070 spin speed versus thicknessApproximate graph readings. Merck, AZ nLOF 2000 Series technical datasheet; p. 1, spin curves. https://www.microchemicals.com/dokumente/datenblaetter/tds/merck/en/tds_az_nlof2000_series.pdf. 150 mm silicon. Final spin duration is not stated. Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.AZ nLOF 2070Approximate graph readings · AZ manufacturer reference03.166.329.4912.61000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

150 mm silicon. Final spin duration is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
100011
20007.6
30006.15
40005.3

Acceleration, exhaust and exact thickness measurement stage are not stated for this curve. Confirm the current supplier process.

Do not automatically identify the applications tag AZ2070 with this nLOF grade; verify the source’s full product name.

Source: Merck, AZ nLOF 2000 Series technical datasheet. p. 1, spin curves. Source checked November 24, 2026.

Original source
Approximate graph readings

SPR220-3.0 · 100 mm

2.3–4.6 µm across 1500–6000 rpm · approximate

SPR220-3.0 · 100 mm spin speed versus thicknessApproximate graph readings. Dow, MEGAPOSIT SPR220 technical datasheet (hosted by UNM); p. 4, Figure 3. https://www.chtm.unm.edu/common/documents/cleanroom-sds/spr-220-data-sheet-r-and-h.pdf. 4-inch wafers (nominal 100 mm). The datasheet specifies thickness-dependent 115 °C soft baking; the final spin time is not stated. Acceleration, dispense, exhaust and curve-specific bake duration are not fully reported. These are approximate readings of Figure 3.SPR220-3.0 · 100 mmApproximate graph readings · SPR manufacturer reference01.322.643.975.29150020003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

4-inch wafers (nominal 100 mm). The datasheet specifies thickness-dependent 115 °C soft baking; the final spin time is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
15004.6
20004
30003.2
40002.8
60002.3

Acceleration, dispense, exhaust and curve-specific bake duration are not fully reported. These are approximate readings of Figure 3.

Source: Dow, MEGAPOSIT SPR220 technical datasheet (hosted by UNM). p. 4, Figure 3. March 2014, Rev. 5; checked November 24, 2026.

Approximate graph readings

SPR220-4.5 · 100 mm

3.4–6.8 µm across 1500–6000 rpm · approximate

SPR220-4.5 · 100 mm spin speed versus thicknessApproximate graph readings. Dow, MEGAPOSIT SPR220 technical datasheet (hosted by UNM); p. 4, Figure 3. https://www.chtm.unm.edu/common/documents/cleanroom-sds/spr-220-data-sheet-r-and-h.pdf. 4-inch wafers (nominal 100 mm). The datasheet specifies thickness-dependent 115 °C soft baking; the final spin time is not stated. Acceleration, dispense, exhaust and curve-specific bake duration are not fully reported. These are approximate readings of Figure 3.SPR220-4.5 · 100 mmApproximate graph readings · SPR manufacturer reference01.953.915.867.82150020003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

4-inch wafers (nominal 100 mm). The datasheet specifies thickness-dependent 115 °C soft baking; the final spin time is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
15006.8
20005.9
30004.7
40004.1
60003.4

Acceleration, dispense, exhaust and curve-specific bake duration are not fully reported. These are approximate readings of Figure 3.

Source: Dow, MEGAPOSIT SPR220 technical datasheet (hosted by UNM). p. 4, Figure 3. March 2014, Rev. 5; checked November 24, 2026.

Approximate graph readings

SPR220-7.0 · 100 mm

5.4–10.2 µm across 1500–6000 rpm · approximate

SPR220-7.0 · 100 mm spin speed versus thicknessApproximate graph readings. Dow, MEGAPOSIT SPR220 technical datasheet (hosted by UNM); p. 4, Figure 3. https://www.chtm.unm.edu/common/documents/cleanroom-sds/spr-220-data-sheet-r-and-h.pdf. 4-inch wafers (nominal 100 mm). The datasheet specifies thickness-dependent 115 °C soft baking; the final spin time is not stated. Acceleration, dispense, exhaust and curve-specific bake duration are not fully reported. These are approximate readings of Figure 3.SPR220-7.0 · 100 mmApproximate graph readings · SPR manufacturer reference02.935.868.811.7150020003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

4-inch wafers (nominal 100 mm). The datasheet specifies thickness-dependent 115 °C soft baking; the final spin time is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
150010.2
20009
30007.5
40006.5
60005.4

Acceleration, dispense, exhaust and curve-specific bake duration are not fully reported. These are approximate readings of Figure 3.

Source: Dow, MEGAPOSIT SPR220 technical datasheet (hosted by UNM). p. 4, Figure 3. March 2014, Rev. 5; checked November 24, 2026.

Approximate graph readings

SPR220-7.0 · 200 mm

8.2–22 µm across 500–2500 rpm · approximate

SPR220-7.0 · 200 mm spin speed versus thicknessApproximate graph readings. Dow, MEGAPOSIT SPR220 technical datasheet (hosted by UNM); p. 4, Figure 4. https://www.chtm.unm.edu/common/documents/cleanroom-sds/spr-220-data-sheet-r-and-h.pdf. 8-inch (200 mm) wafers; SPR220-7.0. Final spin time is not stated. This is a separate published 200 mm reference, not a conversion of the 4-inch curve. Dispense, acceleration and exhaust are not specified.SPR220-7.0 · 200 mmApproximate graph readings · SPR manufacturer reference06.3212.61925.3500100020002500Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

8-inch (200 mm) wafers; SPR220-7.0. Final spin time is not stated.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
50022
100013.8
150010.5
20009
25008.2

This is a separate published 200 mm reference, not a conversion of the 4-inch curve. Dispense, acceleration and exhaust are not specified.

Source: Dow, MEGAPOSIT SPR220 technical datasheet (hosted by UNM). p. 4, Figure 4. March 2014, Rev. 5; checked November 24, 2026.

Approximate graph readings

SPR955-CM-0.9

0.71–1.6 µm across 1000–5000 rpm · approximate

SPR955-CM-0.9 spin speed versus thicknessApproximate graph readings. Rohm and Haas, MEGAPOSIT SPR955-CM datasheet (hosted by Penn State); p. 2, Figure 5. https://www.mri.psu.edu/sites/default/files/docs/LithoDataSheets/Shipley_SPR955_Datasheet.pdf. SPR955-CM grade-specific spin curves. Source thickness values in Å were converted to µm. Wafer diameter, spin time, dispense, exhaust and curve-specific bake are not identified in the curve panel. Original graphics are not reproduced.SPR955-CM-0.9Approximate graph readings · SPR manufacturer reference00.460.921.381.8410002000300040005000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

SPR955-CM grade-specific spin curves. Source thickness values in Å were converted to µm.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10001.6
20001.13
30000.92
40000.8
50000.71

Wafer diameter, spin time, dispense, exhaust and curve-specific bake are not identified in the curve panel. Original graphics are not reproduced.

Source: Rohm and Haas, MEGAPOSIT SPR955-CM datasheet (hosted by Penn State). p. 2, Figure 5. July 2006, Rev. 0; checked November 24, 2026.

Original source
Approximate graph readings

SPR955-CM-1.8

1.43–3.2 µm across 1000–5000 rpm · approximate

SPR955-CM-1.8 spin speed versus thicknessApproximate graph readings. Rohm and Haas, MEGAPOSIT SPR955-CM datasheet (hosted by Penn State); p. 2, Figure 5. https://www.mri.psu.edu/sites/default/files/docs/LithoDataSheets/Shipley_SPR955_Datasheet.pdf. SPR955-CM grade-specific spin curves. Source thickness values in Å were converted to µm. Wafer diameter, spin time, dispense, exhaust and curve-specific bake are not identified in the curve panel. Original graphics are not reproduced.SPR955-CM-1.8Approximate graph readings · SPR manufacturer reference00.921.842.763.6810002000300040005000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

SPR955-CM grade-specific spin curves. Source thickness values in Å were converted to µm.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10003.2
20002.25
30001.85
40001.6
50001.43

Wafer diameter, spin time, dispense, exhaust and curve-specific bake are not identified in the curve panel. Original graphics are not reproduced.

Source: Rohm and Haas, MEGAPOSIT SPR955-CM datasheet (hosted by Penn State). p. 2, Figure 5. July 2006, Rev. 0; checked November 24, 2026.

Original source
Approximate graph readings

SU-8 2000.5

0.5–0.75 µm across 1000–3000 rpm · approximate

SU-8 2000.5 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU); p. 2, Figures 1.a and 1.b; https://labadviser.nanolab.dtu.dk/images/c/c9/SU-8_DataSheet_2005.pdf. Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s). The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.SU-8 2000.5Approximate graph readings · archived manufacturer reference00.2160.4310.6470.862100020003000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s).

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10000.75
20000.57
30000.5

The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.

Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU). p. 2, Figures 1.a and 1.b. Archived document; filename identifies 2005.

Approximate graph readings

SU-8 2002

2–2.9 µm across 1000–3000 rpm · approximate

SU-8 2002 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU); p. 2, Figures 1.a and 1.b; https://labadviser.nanolab.dtu.dk/images/c/c9/SU-8_DataSheet_2005.pdf. Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s). The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.SU-8 2002Approximate graph readings · archived manufacturer reference00.8341.672.53.33100020003000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s).

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10002.9
20002.3
30002

The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.

Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU). p. 2, Figures 1.a and 1.b. Archived document; filename identifies 2005.

Approximate graph readings

SU-8 2005

4.5–7.5 µm across 1000–4000 rpm · approximate

SU-8 2005 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU); p. 2, Figures 1.a and 1.b; https://labadviser.nanolab.dtu.dk/images/c/c9/SU-8_DataSheet_2005.pdf. Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s). The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.SU-8 2005Approximate graph readings · archived manufacturer reference02.164.316.478.631000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s).

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10007.5
20005.7
30005
40004.5

The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.

Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU). p. 2, Figures 1.a and 1.b. Archived document; filename identifies 2005.

Approximate graph readings

SU-8 2007

6–12.5 µm across 1000–4000 rpm · approximate

SU-8 2007 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU); p. 2, Figures 1.a and 1.b; https://labadviser.nanolab.dtu.dk/images/c/c9/SU-8_DataSheet_2005.pdf. Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s). The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.SU-8 2007Approximate graph readings · archived manufacturer reference03.597.1910.814.41000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s).

Data, conditions and source
Reference data (µm)
rpmThickness ≈
100012.5
20008.3
30007
40006

The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.

Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU). p. 2, Figures 1.a and 1.b. Archived document; filename identifies 2005.

Approximate graph readings

SU-8 2010

9–20.5 µm across 1000–4000 rpm · approximate

SU-8 2010 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU); p. 2, Figures 1.a and 1.b; https://labadviser.nanolab.dtu.dk/images/c/c9/SU-8_DataSheet_2005.pdf. Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s). The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.SU-8 2010Approximate graph readings · archived manufacturer reference05.8911.817.723.61000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s).

Data, conditions and source
Reference data (µm)
rpmThickness ≈
100020.5
200013
300010.5
40009

The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.

Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU). p. 2, Figures 1.a and 1.b. Archived document; filename identifies 2005.

Approximate graph readings

SU-8 2015

13–38 µm across 1000–4000 rpm · approximate

SU-8 2015 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU); p. 2, Figures 1.a and 1.b; https://labadviser.nanolab.dtu.dk/images/c/c9/SU-8_DataSheet_2005.pdf. Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s). The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.SU-8 2015Approximate graph readings · archived manufacturer reference010.921.832.843.71000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Guideline: spread at 500 rpm for 5–10 s (100 rpm/s), then final spin for 30 s (300 rpm/s).

Data, conditions and source
Reference data (µm)
rpmThickness ≈
100038
200021
300015.5
400013

The figure does not specify the substrate, exhaust, ambient conditions or exact thickness measurement stage. Confirm the current supplier guidance.

Source: MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU). p. 2, Figures 1.a and 1.b. Archived document; filename identifies 2005.

Approximate graph readings

KMPR 1005

4.5–9.5 µm across 1000–4000 rpm · approximate

KMPR 1005 spin speed versus thicknessApproximate graph readings. Kayaku Advanced Materials, KMPR 1000 product page; Coat section and thickness-versus-spin-speed panel. https://kayakuam.com/product/structsure/kmpr-1000. Guideline: 500 rpm spread for 5–10 s at 100 rpm/s; final spin 30 s at 300 rpm/s. Substrate dimensions, ambient temperature, exhaust and exact measurement stage are not stated on the current curve panel.KMPR 1005Approximate graph readings · Kayaku manufacturer reference02.735.468.1910.91000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Guideline: 500 rpm spread for 5–10 s at 100 rpm/s; final spin 30 s at 300 rpm/s.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10009.5
20006.8
30005.5
40004.5

Substrate dimensions, ambient temperature, exhaust and exact measurement stage are not stated on the current curve panel.

Source: Kayaku Advanced Materials, KMPR 1000 product page. Coat section and thickness-versus-spin-speed panel. Source checked November 24, 2026.

Approximate graph readings

KMPR 1010

11–27 µm across 1000–4000 rpm · approximate

KMPR 1010 spin speed versus thicknessApproximate graph readings. Kayaku Advanced Materials, KMPR 1000 product page; Coat section and thickness-versus-spin-speed panel. https://kayakuam.com/product/structsure/kmpr-1000. Guideline: 500 rpm spread for 5–10 s at 100 rpm/s; final spin 30 s at 300 rpm/s. Substrate dimensions, ambient temperature, exhaust and exact measurement stage are not stated on the current curve panel.KMPR 1010Approximate graph readings · Kayaku manufacturer reference07.7615.523.3311000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Guideline: 500 rpm spread for 5–10 s at 100 rpm/s; final spin 30 s at 300 rpm/s.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
100027
200017
300013
400011

Substrate dimensions, ambient temperature, exhaust and exact measurement stage are not stated on the current curve panel.

Source: Kayaku Advanced Materials, KMPR 1000 product page. Coat section and thickness-versus-spin-speed panel. Source checked November 24, 2026.

Approximate graph readings

KMPR 1025

25–87 µm across 1000–4000 rpm · approximate

KMPR 1025 spin speed versus thicknessApproximate graph readings. Kayaku Advanced Materials, KMPR 1000 product page; Coat section and thickness-versus-spin-speed panel. https://kayakuam.com/product/structsure/kmpr-1000. Guideline: 500 rpm spread for 5–10 s at 100 rpm/s; final spin 30 s at 300 rpm/s. Substrate dimensions, ambient temperature, exhaust and exact measurement stage are not stated on the current curve panel.KMPR 1025Approximate graph readings · Kayaku manufacturer reference02550751001000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Guideline: 500 rpm spread for 5–10 s at 100 rpm/s; final spin 30 s at 300 rpm/s.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
100087
200047
300032
400025

Substrate dimensions, ambient temperature, exhaust and exact measurement stage are not stated on the current curve panel.

Source: Kayaku Advanced Materials, KMPR 1000 product page. Coat section and thickness-versus-spin-speed panel. Source checked November 24, 2026.

Approximate graph readings

KMPR 1050

43–90 µm across 2000–4000 rpm · approximate

KMPR 1050 spin speed versus thicknessApproximate graph readings. Kayaku Advanced Materials, KMPR 1000 product page; Coat section and thickness-versus-spin-speed panel. https://kayakuam.com/product/structsure/kmpr-1000. Guideline: 500 rpm spread for 5–10 s at 100 rpm/s; final spin 30 s at 300 rpm/s. Substrate dimensions, ambient temperature, exhaust and exact measurement stage are not stated on the current curve panel.KMPR 1050Approximate graph readings · Kayaku manufacturer reference025.951.777.6103200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Guideline: 500 rpm spread for 5–10 s at 100 rpm/s; final spin 30 s at 300 rpm/s.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
200090
300059
400043

Substrate dimensions, ambient temperature, exhaust and exact measurement stage are not stated on the current curve panel.

Source: Kayaku Advanced Materials, KMPR 1000 product page. Coat section and thickness-versus-spin-speed panel. Source checked November 24, 2026.

Approximate graph readings

LOR 3A

270–490 nm across 1000–4000 rpm · approximate

LOR 3A spin speed versus thicknessApproximate graph readings. Kayaku Advanced Materials, LOR/PMGI Technical Data Sheet Rev. B (hosted by UBC); pp. 5–6, technical data curves. https://nanofab.sites.olt.ubc.ca/files/2021/01/KAM-LOR-PMGI-Data-Sheet-11719.pdf. Recommended coating: 5 mL on 150 mm silicon; dynamic dispense at 300–500 rpm for 3–5 s; acceleration 10,000 rpm/s; spin 45 s. Specific bake and exhaust used for each curve are not identified. Å values were converted to nm or µm; these are approximate visual readings.LOR 3AApproximate graph readings · Kayaku manufacturer reference01412824235641000200030004000Spin speed (rpm)Film thickness (nm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Recommended coating: 5 mL on 150 mm silicon; dynamic dispense at 300–500 rpm for 3–5 s; acceleration 10,000 rpm/s; spin 45 s.

Data, conditions and source
Reference data (nm)
rpmThickness ≈
1000490
2000350
3000300
4000270

Specific bake and exhaust used for each curve are not identified. Å values were converted to nm or µm; these are approximate visual readings.

Source: Kayaku Advanced Materials, LOR/PMGI Technical Data Sheet Rev. B (hosted by UBC). pp. 5–6, technical data curves. Rev. B, November 2019; checked November 24, 2026.

Original source
Approximate graph readings

LOR 10B

0.85–1.85 µm across 1000–4000 rpm · approximate

LOR 10B spin speed versus thicknessApproximate graph readings. Kayaku Advanced Materials, LOR/PMGI Technical Data Sheet Rev. B (hosted by UBC); pp. 5–6, technical data curves. https://nanofab.sites.olt.ubc.ca/files/2021/01/KAM-LOR-PMGI-Data-Sheet-11719.pdf. Recommended coating: 5 mL on 150 mm silicon; dynamic dispense at 300–500 rpm for 3–5 s; acceleration 10,000 rpm/s; spin 45 s. Specific bake and exhaust used for each curve are not identified. Å values were converted to nm or µm; these are approximate visual readings.LOR 10BApproximate graph readings · Kayaku manufacturer reference00.5321.061.62.131000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Recommended coating: 5 mL on 150 mm silicon; dynamic dispense at 300–500 rpm for 3–5 s; acceleration 10,000 rpm/s; spin 45 s.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10001.85
20001.3
30001
40000.85

Specific bake and exhaust used for each curve are not identified. Å values were converted to nm or µm; these are approximate visual readings.

Source: Kayaku Advanced Materials, LOR/PMGI Technical Data Sheet Rev. B (hosted by UBC). pp. 5–6, technical data curves. Rev. B, November 2019; checked November 24, 2026.

Approximate graph readings

LOR 30B

2.6–4.4 µm across 1000–4000 rpm · approximate

LOR 30B spin speed versus thicknessApproximate graph readings. Kayaku Advanced Materials, LOR/PMGI Technical Data Sheet Rev. B (hosted by UBC); pp. 5–6, technical data curves. https://nanofab.sites.olt.ubc.ca/files/2021/01/KAM-LOR-PMGI-Data-Sheet-11719.pdf. Recommended coating: 5 mL on 150 mm silicon; dynamic dispense at 300–500 rpm for 3–5 s; acceleration 10,000 rpm/s; spin 45 s. Specific bake and exhaust used for each curve are not identified. Å values were converted to nm or µm; these are approximate visual readings.LOR 30BApproximate graph readings · Kayaku manufacturer reference01.262.533.795.061000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Recommended coating: 5 mL on 150 mm silicon; dynamic dispense at 300–500 rpm for 3–5 s; acceleration 10,000 rpm/s; spin 45 s.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10004.4
20003.35
30002.9
40002.6

Specific bake and exhaust used for each curve are not identified. Å values were converted to nm or µm; these are approximate visual readings.

Source: Kayaku Advanced Materials, LOR/PMGI Technical Data Sheet Rev. B (hosted by UBC). pp. 5–6, technical data curves. Rev. B, November 2019; checked November 24, 2026.

Original source
Approximate graph readings

PMGI SF 6

250–480 nm across 1000–4000 rpm · approximate

PMGI SF 6 spin speed versus thicknessApproximate graph readings. Kayaku Advanced Materials, LOR/PMGI Technical Data Sheet Rev. B (hosted by UBC); pp. 5–6, technical data curves. https://nanofab.sites.olt.ubc.ca/files/2021/01/KAM-LOR-PMGI-Data-Sheet-11719.pdf. Recommended coating: 5 mL on 150 mm silicon; dynamic dispense at 300–500 rpm for 3–5 s; acceleration 10,000 rpm/s; spin 45 s. Specific bake and exhaust used for each curve are not identified. Å values were converted to nm or µm; these are approximate visual readings.PMGI SF 6Approximate graph readings · Kayaku manufacturer reference01382764145521000200030004000Spin speed (rpm)Film thickness (nm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Recommended coating: 5 mL on 150 mm silicon; dynamic dispense at 300–500 rpm for 3–5 s; acceleration 10,000 rpm/s; spin 45 s.

Data, conditions and source
Reference data (nm)
rpmThickness ≈
1000480
2000340
3000280
4000250

Specific bake and exhaust used for each curve are not identified. Å values were converted to nm or µm; these are approximate visual readings.

Source: Kayaku Advanced Materials, LOR/PMGI Technical Data Sheet Rev. B (hosted by UBC). pp. 5–6, technical data curves. Rev. B, November 2019; checked November 24, 2026.

Original source
Approximate graph readings

PMGI SF 9

0.47–0.91 µm across 1000–4000 rpm · approximate

PMGI SF 9 spin speed versus thicknessApproximate graph readings. Kayaku Advanced Materials, LOR/PMGI Technical Data Sheet Rev. B (hosted by UBC); pp. 5–6, technical data curves. https://nanofab.sites.olt.ubc.ca/files/2021/01/KAM-LOR-PMGI-Data-Sheet-11719.pdf. Recommended coating: 5 mL on 150 mm silicon; dynamic dispense at 300–500 rpm for 3–5 s; acceleration 10,000 rpm/s; spin 45 s. Specific bake and exhaust used for each curve are not identified. Å values were converted to nm or µm; these are approximate visual readings.PMGI SF 9Approximate graph readings · Kayaku manufacturer reference00.2620.5230.7851.051000200030004000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Recommended coating: 5 mL on 150 mm silicon; dynamic dispense at 300–500 rpm for 3–5 s; acceleration 10,000 rpm/s; spin 45 s.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10000.91
20000.65
30000.54
40000.47

Specific bake and exhaust used for each curve are not identified. Å values were converted to nm or µm; these are approximate visual readings.

Source: Kayaku Advanced Materials, LOR/PMGI Technical Data Sheet Rev. B (hosted by UBC). pp. 5–6, technical data curves. Rev. B, November 2019; checked November 24, 2026.

Original source
Published lab fit

PMMA 950K A2

10–81.4 nm across 1000–6000 rpm

PMMA 950K A2 spin speed versus film thicknessPublished lab fit. Thickness in nm. Source: MIT.nano, Electron-beam lithography: resists; PMMA and HSQ spin-curve panels; published exponential fits; https://nanousers.mit.edu/ebl/resists. Small samples; spread 750 rpm for 5 s; accelerate 10,000 rpm/s; final spin 60 s. PMMA: bake 180 °C for 120 s. HSQ: bake 90 °C for 120 s. Exact sample dimensions and ambient/exhaust conditions are not reported. Values come from the lab’s fitted equations, not raw measurements; fit uncertainty is not reproduced.PMMA 950K A2Published lab fit · MIT.nano023.446.870.293.6100020003000400050006000Spin speed (rpm)Film thickness (nm)Line: published fit evaluated within displayed range.Cee® original plot · Source details accompany this chart · Starting reference

Small samples; spread 750 rpm for 5 s; accelerate 10,000 rpm/s; final spin 60 s. PMMA: bake 180 °C for 120 s. HSQ: bake 90 °C for 120 s.

Data, conditions and source
Values evaluated from the published fit (nm)
rpmThickness
100081.4
200043.8
300025.4
400016.5
500012.2
600010

Published fit: h (nm) = 150.6 × exp[−(rpm/1000)/1.39] + 8.04. Displayed range: 1000–6000 rpm. Fit evaluations are not measured data points.

View original source panel

Exact sample dimensions and ambient/exhaust conditions are not reported. Values come from the lab’s fitted equations, not raw measurements; fit uncertainty is not reproduced.

Source: MIT.nano, Electron-beam lithography: resists. PMMA and HSQ spin-curve panels; published exponential fits. Measurement date not stated; accessed November 24, 2026.

Published lab fit

PMMA 950K A4

89.8–382.3 nm across 1000–6000 rpm

PMMA 950K A4 spin speed versus film thicknessPublished lab fit. Thickness in nm. Source: MIT.nano, Electron-beam lithography: resists; PMMA and HSQ spin-curve panels; published exponential fits; https://nanousers.mit.edu/ebl/resists. Small samples; spread 750 rpm for 5 s; accelerate 10,000 rpm/s; final spin 60 s. PMMA: bake 180 °C for 120 s. HSQ: bake 90 °C for 120 s. Exact sample dimensions and ambient/exhaust conditions are not reported. Values come from the lab’s fitted equations, not raw measurements; fit uncertainty is not reproduced.PMMA 950K A4Published lab fit · MIT.nano0110220330440100020003000400050006000Spin speed (rpm)Film thickness (nm)Line: published fit evaluated within displayed range.Cee® original plot · Source details accompany this chart · Starting reference

Small samples; spread 750 rpm for 5 s; accelerate 10,000 rpm/s; final spin 60 s. PMMA: bake 180 °C for 120 s. HSQ: bake 90 °C for 120 s.

Data, conditions and source
Values evaluated from the published fit (nm)
rpmThickness
1000382.3
2000246.1
3000169.8
4000127.1
5000103.2
600089.8

Published fit: h (nm) = 552.7 × exp[−(rpm/1000)/1.724] + 72.82. Displayed range: 1000–6000 rpm. Fit evaluations are not measured data points.

View original source panel

Exact sample dimensions and ambient/exhaust conditions are not reported. Values come from the lab’s fitted equations, not raw measurements; fit uncertainty is not reproduced.

Source: MIT.nano, Electron-beam lithography: resists. PMMA and HSQ spin-curve panels; published exponential fits. Measurement date not stated; accessed November 24, 2026.

Published lab measurements

PMMA AR-P 672.03 · 1:1 anisole

28.76–51.37 nm across 2000–7000 rpm

PMMA AR-P 672.03 · 1:1 anisole spin speed versus film thicknessPublished lab measurements. Thickness in nm. Source: DTU Nanolab, LabAdviser: PMMA; Spin Curves tables; https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/PMMA&oldid=51698. ~2 mL on 4-inch silicon wafers; acceleration 2000 rpm/s; bake 150 °C for 3 min. Ellipsometry at nine locations. Final spin duration is not reported. These are DTU facility results, not Cee equipment validation.PMMA AR-P 672.03 · 1:1 anisolePublished lab measurements · DTU Nanolab014.829.544.359.1200030004000500060007000Spin speed (rpm)Film thickness (nm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

~2 mL on 4-inch silicon wafers; acceleration 2000 rpm/s; bake 150 °C for 3 min. Ellipsometry at nine locations.

Data, conditions and source

Allresist AR-P 672.03 diluted 1:1 in anisole; source does not specify ratio basis

Reference data (nm)
rpmThicknessSpatial SD
200051.370.25
300041.970.24
400036.250.25
500032.420.3
600030.170.29
700028.760.43

SD is variation across nine wafer locations, not overall process uncertainty.

Final spin duration is not reported. These are DTU facility results, not Cee equipment validation.

Source: DTU Nanolab, LabAdviser: PMMA. Spin Curves tables. Measurements: October 26, 2015; page revision: May 5, 2025.

Published lab measurements

PMMA AR-P 672.03 · as supplied

72.79–95.55 nm across 4000–7000 rpm

PMMA AR-P 672.03 · as supplied spin speed versus film thicknessPublished lab measurements. Thickness in nm. Source: DTU Nanolab, LabAdviser: PMMA; Spin Curves tables; https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/PMMA&oldid=51698. ~2 mL on 4-inch silicon wafers; acceleration 2000 rpm/s; bake 150 °C for 3 min. Ellipsometry at nine locations. Final spin duration is not reported. These are DTU facility results, not Cee equipment validation.PMMA AR-P 672.03 · as suppliedPublished lab measurements · DTU Nanolab027.554.982.41104000500060007000Spin speed (rpm)Film thickness (nm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

~2 mL on 4-inch silicon wafers; acceleration 2000 rpm/s; bake 150 °C for 3 min. Ellipsometry at nine locations.

Data, conditions and source

Allresist AR-P 672.03, as supplied

Reference data (nm)
rpmThicknessSpatial SD
400095.550.55
500085.50.92
700072.791.18

SD is variation across nine wafer locations, not overall process uncertainty.

Final spin duration is not reported. These are DTU facility results, not Cee equipment validation.

Source: DTU Nanolab, LabAdviser: PMMA. Spin Curves tables. Measurements: October 26, 2015; page revision: May 5, 2025.

Published research fit

PDMS Sylgard 184 · 33 wt% in TBA

3.28–6.15 µm across 1000–6000 rpm

PDMS Sylgard 184 · 33 wt% in TBA spin speed versus thicknessPublished research fit. Koschwanez, Carlson & Meldrum (2009), Thin PDMS Films Using Long Spin Times or Tert-Butyl Alcohol as a Solvent; Figure 2, Equation 1 and Table 2. https://journals.plos.org/plosone/article?id=10.1371/journal.pone.0004572. Sylgard 184 base:curing agent 10:1 by weight; glass slides; 5 min spin, beginning 15 min after mixing; cure at 60 °C for 1–2 h. Mixture age, dilution and substrate matter. These fits are for the paper’s glass-substrate process; confidence intervals are not reproduced.PDMS Sylgard 184 · 33 wt% in TBAPublished research fit · Koschwanez et al., 200901.773.545.37.07100020003000400050006000Spin speed (rpm)Film thickness (µm)Line: published fit evaluated within displayed range.Cee® original plot · Source details accompany this chart · Starting reference

Sylgard 184 base:curing agent 10:1 by weight; glass slides; 5 min spin, beginning 15 min after mixing; cure at 60 °C for 1–2 h.

Data, conditions and source

Mixed Sylgard 184 (base:curing agent 10:1 by mass), diluted to 33 wt% PDMS in tert-butyl alcohol

Evaluated published fit (µm)
rpmThickness
10006.15
20004.82
30004.19
40003.79
50003.5
60003.28

Published fit: h (µm) = 69 × rpm^(-0.35). Table values are rounded evaluations of this fit, not measured data points.

Mixture age, dilution and substrate matter. These fits are for the paper’s glass-substrate process; confidence intervals are not reproduced.

Source: Koschwanez, Carlson & Meldrum (2009), Thin PDMS Films Using Long Spin Times or Tert-Butyl Alcohol as a Solvent. Figure 2, Equation 1 and Table 2. Published February 24, 2009; checked November 24, 2026.

Published research fit

PDMS Sylgard 184 · 50 wt% in TBA

4.11–12.05 µm across 1000–6000 rpm

PDMS Sylgard 184 · 50 wt% in TBA spin speed versus thicknessPublished research fit. Koschwanez, Carlson & Meldrum (2009), Thin PDMS Films Using Long Spin Times or Tert-Butyl Alcohol as a Solvent; Figure 2, Equation 1 and Table 2. https://journals.plos.org/plosone/article?id=10.1371/journal.pone.0004572. Sylgard 184 base:curing agent 10:1 by weight; glass slides; 5 min spin, beginning 15 min after mixing; cure at 60 °C for 1–2 h. Mixture age, dilution and substrate matter. These fits are for the paper’s glass-substrate process; confidence intervals are not reproduced.PDMS Sylgard 184 · 50 wt% in TBAPublished research fit · Koschwanez et al., 200903.466.9310.413.9100020003000400050006000Spin speed (rpm)Film thickness (µm)Line: published fit evaluated within displayed range.Cee® original plot · Source details accompany this chart · Starting reference

Sylgard 184 base:curing agent 10:1 by weight; glass slides; 5 min spin, beginning 15 min after mixing; cure at 60 °C for 1–2 h.

Data, conditions and source

Mixed Sylgard 184 (base:curing agent 10:1 by mass), diluted to 50 wt% PDMS in tert-butyl alcohol

Evaluated published fit (µm)
rpmThickness
100012.05
20007.95
30006.23
40005.24
50004.59
60004.11

Published fit: h (µm) = 760 × rpm^(-0.6). Table values are rounded evaluations of this fit, not measured data points.

Mixture age, dilution and substrate matter. These fits are for the paper’s glass-substrate process; confidence intervals are not reproduced.

Source: Koschwanez, Carlson & Meldrum (2009), Thin PDMS Films Using Long Spin Times or Tert-Butyl Alcohol as a Solvent. Figure 2, Equation 1 and Table 2. Published February 24, 2009; checked November 24, 2026.

Published research fit

PDMS Sylgard 184 · undiluted

4.36–25.26 µm across 1000–6000 rpm

PDMS Sylgard 184 · undiluted spin speed versus thicknessPublished research fit. Koschwanez, Carlson & Meldrum (2009), Thin PDMS Films Using Long Spin Times or Tert-Butyl Alcohol as a Solvent; Figure 2, Equation 1 and Table 2. https://journals.plos.org/plosone/article?id=10.1371/journal.pone.0004572. Sylgard 184 base:curing agent 10:1 by weight; glass slides; 5 min spin, beginning 15 min after mixing; cure at 60 °C for 1–2 h. Mixture age, dilution and substrate matter. These fits are for the paper’s glass-substrate process; confidence intervals are not reproduced.PDMS Sylgard 184 · undilutedPublished research fit · Koschwanez et al., 200907.2614.521.829100020003000400050006000Spin speed (rpm)Film thickness (µm)Line: published fit evaluated within displayed range.Cee® original plot · Source details accompany this chart · Starting reference

Sylgard 184 base:curing agent 10:1 by weight; glass slides; 5 min spin, beginning 15 min after mixing; cure at 60 °C for 1–2 h.

Data, conditions and source

Sylgard 184 base:curing agent 10:1 by mass; no TBA dilution

Evaluated published fit (µm)
rpmThickness
100025.26
200012.81
30008.61
40006.49
50005.22
60004.36

Published fit: h (µm) = 22000 × rpm^(-0.98). Table values are rounded evaluations of this fit, not measured data points.

Mixture age, dilution and substrate matter. These fits are for the paper’s glass-substrate process; confidence intervals are not reproduced.

Source: Koschwanez, Carlson & Meldrum (2009), Thin PDMS Films Using Long Spin Times or Tert-Butyl Alcohol as a Solvent. Figure 2, Equation 1 and Table 2. Published February 24, 2009; checked November 24, 2026.

Published lab fit

HSQ 2%

16.7–58.6 nm across 1000–6000 rpm

HSQ 2% spin speed versus film thicknessPublished lab fit. Thickness in nm. Source: MIT.nano, Electron-beam lithography: resists; PMMA and HSQ spin-curve panels; published exponential fits; https://nanousers.mit.edu/ebl/resists. Small samples; spread 750 rpm for 5 s; accelerate 10,000 rpm/s; final spin 60 s. PMMA: bake 180 °C for 120 s. HSQ: bake 90 °C for 120 s. Exact sample dimensions and ambient/exhaust conditions are not reported. Values come from the lab’s fitted equations, not raw measurements; fit uncertainty is not reproduced.HSQ 2%Published lab fit · MIT.nano016.833.750.567.4100020003000400050006000Spin speed (rpm)Film thickness (nm)Line: published fit evaluated within displayed range.Cee® original plot · Source details accompany this chart · Starting reference

Small samples; spread 750 rpm for 5 s; accelerate 10,000 rpm/s; final spin 60 s. PMMA: bake 180 °C for 120 s. HSQ: bake 90 °C for 120 s.

Data, conditions and source
Values evaluated from the published fit (nm)
rpmThickness
100058.6
200042.5
300031.8
400024.6
500019.9
600016.7

Published fit: h (nm) = 72.46 × exp[−(rpm/1000)/2.46] + 10.39. Displayed range: 1000–6000 rpm. Fit evaluations are not measured data points.

View original source panel

Exact sample dimensions and ambient/exhaust conditions are not reported. Values come from the lab’s fitted equations, not raw measurements; fit uncertainty is not reproduced.

Source: MIT.nano, Electron-beam lithography: resists. PMMA and HSQ spin-curve panels; published exponential fits. Measurement date not stated; accessed November 24, 2026.

Published lab fit

HSQ 4%

42.4–148 nm across 1000–6000 rpm

HSQ 4% spin speed versus film thicknessPublished lab fit. Thickness in nm. Source: MIT.nano, Electron-beam lithography: resists; PMMA and HSQ spin-curve panels; published exponential fits; https://nanousers.mit.edu/ebl/resists. Small samples; spread 750 rpm for 5 s; accelerate 10,000 rpm/s; final spin 60 s. PMMA: bake 180 °C for 120 s. HSQ: bake 90 °C for 120 s. Exact sample dimensions and ambient/exhaust conditions are not reported. Values come from the lab’s fitted equations, not raw measurements; fit uncertainty is not reproduced.HSQ 4%Published lab fit · MIT.nano042.585.1128170100020003000400050006000Spin speed (rpm)Film thickness (nm)Line: published fit evaluated within displayed range.Cee® original plot · Source details accompany this chart · Starting reference

Small samples; spread 750 rpm for 5 s; accelerate 10,000 rpm/s; final spin 60 s. PMMA: bake 180 °C for 120 s. HSQ: bake 90 °C for 120 s.

Data, conditions and source
Values evaluated from the published fit (nm)
rpmThickness
1000148
200097.9
300070.3
400055.2
500046.9
600042.4

Published fit: h (nm) = 202.6 × exp[−(rpm/1000)/1.668] + 36.8. Displayed range: 1000–6000 rpm. Fit evaluations are not measured data points.

View original source panel

Exact sample dimensions and ambient/exhaust conditions are not reported. Values come from the lab’s fitted equations, not raw measurements; fit uncertainty is not reproduced.

Source: MIT.nano, Electron-beam lithography: resists. PMMA and HSQ spin-curve panels; published exponential fits. Measurement date not stated; accessed November 24, 2026.

Published lab fit

HSQ 6%

68.6–302.9 nm across 1000–6000 rpm

HSQ 6% spin speed versus film thicknessPublished lab fit. Thickness in nm. Source: MIT.nano, Electron-beam lithography: resists; PMMA and HSQ spin-curve panels; published exponential fits; https://nanousers.mit.edu/ebl/resists. Small samples; spread 750 rpm for 5 s; accelerate 10,000 rpm/s; final spin 60 s. PMMA: bake 180 °C for 120 s. HSQ: bake 90 °C for 120 s. Exact sample dimensions and ambient/exhaust conditions are not reported. Values come from the lab’s fitted equations, not raw measurements; fit uncertainty is not reproduced.HSQ 6%Published lab fit · MIT.nano087.1174261348100020003000400050006000Spin speed (rpm)Film thickness (nm)Line: published fit evaluated within displayed range.Cee® original plot · Source details accompany this chart · Starting reference

Small samples; spread 750 rpm for 5 s; accelerate 10,000 rpm/s; final spin 60 s. PMMA: bake 180 °C for 120 s. HSQ: bake 90 °C for 120 s.

Data, conditions and source
Values evaluated from the published fit (nm)
rpmThickness
1000302.9
2000186.9
3000126
400094.1
500077.4
600068.6

Published fit: h (nm) = 465.2 × exp[−(rpm/1000)/1.55] + 58.88. Displayed range: 1000–6000 rpm. Fit evaluations are not measured data points.

View original source panel

Exact sample dimensions and ambient/exhaust conditions are not reported. Values come from the lab’s fitted equations, not raw measurements; fit uncertainty is not reproduced.

Source: MIT.nano, Electron-beam lithography: resists. PMMA and HSQ spin-curve panels; published exponential fits. Measurement date not stated; accessed November 24, 2026.

Approximate graph readings

S1805 G2

0.4–0.99 µm across 1000–6000 rpm · approximate

S1805 G2 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: micro resist technology, resist selection catalogue (archived supplier document hosted by DTU); p. 4, S1800 G2 graph; https://labadviser.nanolab.dtu.dk/images/6/6e/UVN2300.pdf. Spin duration and acceleration are not stated on the source page. Archived reference with incomplete conditions. Verify grade availability and the current supplier datasheet before choosing a trial.S1805 G2Approximate graph readings · supplier reference00.2850.5690.8541.14100020003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Spin duration and acceleration are not stated on the source page.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10000.99
20000.71
40000.5
60000.4

Archived reference with incomplete conditions. Verify grade availability and the current supplier datasheet before choosing a trial.

Source: micro resist technology, resist selection catalogue (archived supplier document hosted by DTU). p. 4, S1800 G2 graph. Publication date not established.

Approximate graph readings

S1813 G2

1.05–2.5 µm across 1000–6000 rpm · approximate

S1813 G2 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: micro resist technology, resist selection catalogue (archived supplier document hosted by DTU); p. 4, S1800 G2 graph; https://labadviser.nanolab.dtu.dk/images/6/6e/UVN2300.pdf. Spin duration and acceleration are not stated on the source page. Archived reference with incomplete conditions. Verify grade availability and the current supplier datasheet before choosing a trial.S1813 G2Approximate graph readings · supplier reference00.7191.442.162.88100020003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Spin duration and acceleration are not stated on the source page.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10002.5
20001.8
40001.3
60001.05

Archived reference with incomplete conditions. Verify grade availability and the current supplier datasheet before choosing a trial.

Source: micro resist technology, resist selection catalogue (archived supplier document hosted by DTU). p. 4, S1800 G2 graph. Publication date not established.

Approximate graph readings

ma-P 1215

1.05–2.6 µm across 1000–6000 rpm · approximate

ma-P 1215 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: micro resist technology, Positive Photoresists for UV, Laser & Greyscale Lithography; p. 2, upper spin curves; https://www.microresist.de/wp-content/uploads/2022/08/flyer_pos_220831_final.pdf. 30 s final spin, as labeled in the source graph. Substrate, acceleration, exhaust and thickness measurement stage are not specified in the graph.ma-P 1215Approximate graph readings · supplier reference00.7471.492.242.99100020003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

30 s final spin, as labeled in the source graph.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10002.6
20001.8
30001.5
60001.05

Substrate, acceleration, exhaust and thickness measurement stage are not specified in the graph.

Source: micro resist technology, Positive Photoresists for UV, Laser & Greyscale Lithography. p. 2, upper spin curves. August 2022.

Approximate graph readings

ma-P 1225

1.7–4.3 µm across 1000–6000 rpm · approximate

ma-P 1225 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: micro resist technology, Positive Photoresists for UV, Laser & Greyscale Lithography; p. 2, upper spin curves; https://www.microresist.de/wp-content/uploads/2022/08/flyer_pos_220831_final.pdf. 30 s final spin, as labeled in the source graph. Substrate, acceleration, exhaust and thickness measurement stage are not specified in the graph.ma-P 1225Approximate graph readings · supplier reference01.242.473.714.94100020003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

30 s final spin, as labeled in the source graph.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10004.3
20002.95
30002.5
60001.7

Substrate, acceleration, exhaust and thickness measurement stage are not specified in the graph.

Source: micro resist technology, Positive Photoresists for UV, Laser & Greyscale Lithography. p. 2, upper spin curves. August 2022.

Approximate graph readings

ma-P 1240

2.7–7.2 µm across 1000–6000 rpm · approximate

ma-P 1240 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: micro resist technology, Positive Photoresists for UV, Laser & Greyscale Lithography; p. 2, upper spin curves; https://www.microresist.de/wp-content/uploads/2022/08/flyer_pos_220831_final.pdf. 30 s final spin, as labeled in the source graph. Substrate, acceleration, exhaust and thickness measurement stage are not specified in the graph.ma-P 1240Approximate graph readings · supplier reference02.074.146.218.28100020003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

30 s final spin, as labeled in the source graph.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
10007.2
20004.9
30004
60002.7

Substrate, acceleration, exhaust and thickness measurement stage are not specified in the graph.

Source: micro resist technology, Positive Photoresists for UV, Laser & Greyscale Lithography. p. 2, upper spin curves. August 2022.

Approximate graph readings

ma-P 1275

5.1–14.7 µm across 1000–6000 rpm · approximate

ma-P 1275 spin speed versus film thicknessApproximate graph readings. Thickness in µm. Source: micro resist technology, Positive Photoresists for UV, Laser & Greyscale Lithography; p. 2, upper spin curves; https://www.microresist.de/wp-content/uploads/2022/08/flyer_pos_220831_final.pdf. 30 s final spin, as labeled in the source graph. Substrate, acceleration, exhaust and thickness measurement stage are not specified in the graph.ma-P 1275Approximate graph readings · supplier reference04.238.4512.716.9100020003000400050006000Spin speed (rpm)Film thickness (µm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

30 s final spin, as labeled in the source graph.

Data, conditions and source
Reference data (µm)
rpmThickness ≈
100014.7
20009.5
30007.5
60005.1

Substrate, acceleration, exhaust and thickness measurement stage are not specified in the graph.

Source: micro resist technology, Positive Photoresists for UV, Laser & Greyscale Lithography. p. 2, upper spin curves. August 2022.

Approximate graph readings

ZEP520A · 11 mPa·s

310–700 nm across 1000–5000 rpm · approximate

ZEP520A · 11 mPa·s spin speed versus thicknessApproximate graph readings. Zeon Corporation, Electron Beam Resist product information; ZEP520A spin-curve panel. https://www.zeon.co.jp/en/business/enterprise/electronic/imagelec/. Anisole formulations: ZEP520A (11 mPa·s) and ZEP520A-7 (7 mPa·s). Wafer diameter, spin duration, bake and acceleration are not stated on the source panel. These grades are not interchangeable.ZEP520A · 11 mPa·sApproximate graph readings · Zeon manufacturer reference020140260480510002000300040005000Spin speed (rpm)Film thickness (nm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Anisole formulations: ZEP520A (11 mPa·s) and ZEP520A-7 (7 mPa·s).

Data, conditions and source
Reference data (nm)
rpmThickness ≈
1000700
2000500
3000400
4000350
5000310

Wafer diameter, spin duration, bake and acceleration are not stated on the source panel. These grades are not interchangeable.

Source: Zeon Corporation, Electron Beam Resist product information. ZEP520A spin-curve panel. Checked November 24, 2026.

Original source
Approximate graph readings

ZEP520A-7 · 7 mPa·s

200–420 nm across 1000–5000 rpm · approximate

ZEP520A-7 · 7 mPa·s spin speed versus thicknessApproximate graph readings. Zeon Corporation, Electron Beam Resist product information; ZEP520A spin-curve panel. https://www.zeon.co.jp/en/business/enterprise/electronic/imagelec/. Anisole formulations: ZEP520A (11 mPa·s) and ZEP520A-7 (7 mPa·s). Wafer diameter, spin duration, bake and acceleration are not stated on the source panel. These grades are not interchangeable.ZEP520A-7 · 7 mPa·sApproximate graph readings · Zeon manufacturer reference012124136248310002000300040005000Spin speed (rpm)Film thickness (nm)Dots: reference points. Dashed line: log–log interpolation.Cee® original plot · Source details accompany this chart · Starting reference

Anisole formulations: ZEP520A (11 mPa·s) and ZEP520A-7 (7 mPa·s).

Data, conditions and source
Reference data (nm)
rpmThickness ≈
1000420
2000300
3000250
4000220
5000200

Wafer diameter, spin duration, bake and acceleration are not stated on the source panel. These grades are not interchangeable.

Source: Zeon Corporation, Electron Beam Resist product information. ZEP520A spin-curve panel. Checked November 24, 2026.

Original source
Published lab fit

CSAR 62 · AR-P 6200.09

77.3–323.5 nm across 1000–6000 rpm

CSAR 62 · AR-P 6200.09 spin speed versus thicknessPublished lab fit. MIT.nano, Electron-beam lithography: resists; CSAR 62.09 panel, published exponential fit. https://nanousers.mit.edu/ebl/resists. Small samples; spread 750 rpm for 5 s; ramp 10,000 rpm/s; final spin 60 s; bake 150 °C for 120 s. Exact sample dimensions, ambient conditions and exhaust are not stated. Fit values are not raw measurements.CSAR 62 · AR-P 6200.09Published lab fit · MIT.nano lab fit093186279372100020003000400050006000Spin speed (rpm)Film thickness (nm)Line: published fit evaluated within displayed range.Cee® original plot · Source details accompany this chart · Starting reference

Small samples; spread 750 rpm for 5 s; ramp 10,000 rpm/s; final spin 60 s; bake 150 °C for 120 s.

Data, conditions and source
Evaluated published fit (nm)
rpmThickness
1000323.5
2000233.5
3000171.2
4000128
500098.1
600077.3

Published fit: h (nm) = 422.8 × exp[−(rpm/1000)/2.724] + 30.61. Table values are rounded evaluations of this fit, not measured data points.

Exact sample dimensions, ambient conditions and exhaust are not stated. Fit values are not raw measurements.

Source: MIT.nano, Electron-beam lithography: resists. CSAR 62.09 panel, published exponential fit. Checked November 24, 2026.

Original source
Published lab fit

ma-N 2401

36.3–145.5 nm across 1000–6000 rpm

ma-N 2401 spin speed versus thicknessPublished lab fit. MIT.nano, Electron-beam lithography: resists; ma-N 2401 and 2403 panels, published exponential fits. https://nanousers.mit.edu/ebl/resists. Small samples; spread 750 rpm for 5 s; ramp 10,000 rpm/s; final spin 60 s; bake 100 °C for 240 s. Exact sample dimensions, ambient conditions and exhaust are not stated. Fit values are not raw measurements.ma-N 2401Published lab fit · MIT.nano lab fit041.883.7125167100020003000400050006000Spin speed (rpm)Film thickness (nm)Line: published fit evaluated within displayed range.Cee® original plot · Source details accompany this chart · Starting reference

Small samples; spread 750 rpm for 5 s; ramp 10,000 rpm/s; final spin 60 s; bake 100 °C for 240 s.

Data, conditions and source
Evaluated published fit (nm)
rpmThickness
1000145.5
2000101.7
300073.6
400055.5
500043.8
600036.3

Published fit: h (nm) = 190.8 × exp[−(rpm/1000)/2.267] + 22.78. Table values are rounded evaluations of this fit, not measured data points.

Exact sample dimensions, ambient conditions and exhaust are not stated. Fit values are not raw measurements.

Source: MIT.nano, Electron-beam lithography: resists. ma-N 2401 and 2403 panels, published exponential fits. Checked November 24, 2026.

Original source
Published lab fit

ma-N 2403

96.7–368 nm across 1000–6000 rpm

ma-N 2403 spin speed versus thicknessPublished lab fit. MIT.nano, Electron-beam lithography: resists; ma-N 2401 and 2403 panels, published exponential fits. https://nanousers.mit.edu/ebl/resists. Small samples; spread 750 rpm for 5 s; ramp 10,000 rpm/s; final spin 60 s; bake 100 °C for 240 s. Exact sample dimensions, ambient conditions and exhaust are not stated. Fit values are not raw measurements.ma-N 2403Published lab fit · MIT.nano lab fit0106212317423100020003000400050006000Spin speed (rpm)Film thickness (nm)Line: published fit evaluated within displayed range.Cee® original plot · Source details accompany this chart · Starting reference

Small samples; spread 750 rpm for 5 s; ramp 10,000 rpm/s; final spin 60 s; bake 100 °C for 240 s.

Data, conditions and source
Evaluated published fit (nm)
rpmThickness
1000368
2000256.8
3000186.6
4000142.3
5000114.3
600096.7

Published fit: h (nm) = 477.7 × exp[−(rpm/1000)/2.173] + 66.48. Table values are rounded evaluations of this fit, not measured data points.

Exact sample dimensions, ambient conditions and exhaust are not stated. Fit values are not raw measurements.

Source: MIT.nano, Electron-beam lithography: resists. ma-N 2401 and 2403 panels, published exponential fits. Checked November 24, 2026.

Original source

Estimate a starting speed

Use one selected reference within its displayed range. Interpolation adds an estimate between reference points; it does not supply missing process conditions.

Choose a formulation and target thickness to see an estimate.

Single recipe references

These Cee measurements provide a starting example at one speed. They are kept outside the curve estimator because one recipe does not establish a speed–thickness relationship.

AZ 4620 · Cee 300X reference — 2000 rpm / 9.11 µm

300 mm silicon; static dispense 30 mL; spread 500 rpm for 10 s; final spin 60 s at 2000 rpm; acceleration 2000 rpm/s; exhaust 20%, lid ports closed; bake 110 °C for 90 s.

Reported mean thickness; one speed, so no interpolated curve. The report states 0.63% total thickness variation for this experiment.

Cee 300X uniformity report — AZ 4620 section and Table 2.

SU-8 3025 · Cee 300X reference — 1750 rpm / 39.49 µm

300 mm silicon; static dispense 30 mL; spread 500 rpm for 15 s; final spin 45 s at 1750 rpm; final acceleration 1750 rpm/s; exhaust 15%, lid ports closed; bake 95 °C for 13 min.

Reported mean thickness; one speed, so no interpolated curve. The report states 1.81% total thickness variation for this experiment.

Cee 300X uniformity report — SU-8 3025 section and Table 3.

Sources and chart method

Charts use original Cee formatting. Supplier graph values were read visually and rounded; dashed segments use local log–log interpolation. Published measured tables retain their stated precision. MIT curves evaluate published exponential fits; PDMS curves evaluate formulation-specific power-law fits from the cited paper. Both stay within their displayed source range. No curve uses an assumed universal square-root relationship.

  1. MicroChem SU-8 2000 processing guidelines (archived manufacturer document hosted by DTU) — p. 2, Figures 1.a and 1.b. Archived document; filename identifies 2005.
  2. micro resist technology, Positive Photoresists for UV, Laser & Greyscale Lithography — p. 2, upper spin curves. August 2022.
  3. micro resist technology, resist selection catalogue (archived supplier document hosted by DTU) — p. 4, S1800 G2 graph. Publication date not established.
  4. DTU Nanolab, LabAdviser: PMMA — Spin Curves tables. Measurements: October 26, 2015; page revision: May 5, 2025.
  5. MIT.nano, Electron-beam lithography: resists — PMMA and HSQ spin-curve panels; published exponential fits. Measurement date not stated; accessed November 24, 2026.
  6. Merck, AZ 1500 Series technical datasheet — p. 1, spin curves. Source checked November 24, 2026.
  7. Merck, AZ 5214E technical datasheet — p. 2, characteristic thickness table. Source checked November 24, 2026.
  8. Merck, AZ nLOF 2000 Series technical datasheet — p. 1, spin curves. Source checked November 24, 2026.
  9. AZ Electronic Materials, AZ 9260 data package (hosted by University of Utah) — p. 4, film thickness versus spin speed. Source checked November 24, 2026.
  10. Merck, AZ 10XT technical datasheet — p. 1, spin curves; p. 12, coating notes. Revision March 2021; checked November 24, 2026.
  11. Merck, AZ 12XT-20PL technical datasheet — p. 1, spin curve. Source checked November 24, 2026.
  12. Merck, AZ 40XT-11D technical datasheet — p. 1, spin curve. Revision July 2016; checked November 24, 2026.
  13. Merck, AZ MiR 701 Series technical datasheet — p. 1, spin curves. Source checked November 24, 2026.
  14. Clariant/AZ, BARLi II technical brochure — p. 3, film-thickness table. Source checked November 24, 2026.
  15. Kayaku Advanced Materials, KMPR 1000 product page — Coat section and thickness-versus-spin-speed panel. Source checked November 24, 2026.
  16. Kayaku Advanced Materials, LOR/PMGI Technical Data Sheet Rev. B (hosted by UBC) — pp. 5–6, technical data curves. Rev. B, November 2019; checked November 24, 2026.
  17. Koschwanez, Carlson & Meldrum (2009), Thin PDMS Films Using Long Spin Times or Tert-Butyl Alcohol as a Solvent — Figure 2, Equation 1 and Table 2. Published February 24, 2009; checked November 24, 2026.
  18. Dow, MEGAPOSIT SPR220 technical datasheet (hosted by UNM) — p. 4, Figure 3. March 2014, Rev. 5; checked November 24, 2026.
  19. Dow, MEGAPOSIT SPR220 technical datasheet (hosted by UNM) — p. 4, Figure 4. March 2014, Rev. 5; checked November 24, 2026.
  20. Rohm and Haas, MEGAPOSIT SPR955-CM datasheet (hosted by Penn State) — p. 2, Figure 5. July 2006, Rev. 0; checked November 24, 2026.
  21. Zeon Corporation, Electron Beam Resist product information — ZEP520A spin-curve panel. Checked November 24, 2026.
  22. MIT.nano, Electron-beam lithography: resists — CSAR 62.09 panel, published exponential fit. Checked November 24, 2026.
  23. MIT.nano, Electron-beam lithography: resists — ma-N 2401 and 2403 panels, published exponential fits. Checked November 24, 2026.

SEMICON EUROPA · 10–13 NOVEMBER

Bring your process questions.

Meet Jacob, CEE’s Global Sales Director, in Munich with our partner SiSTEM Technology.

Stand C1353 · Messe München
Spin coating, bake and chill, temporary bonding and debonding.

Book a stand meeting →

Mention Jacob from CEE in SiSTEM’s booking form.